Showing all 12 results

Quality from the Czech Republic

COE
info via Simax

33

3,3 .10- 6 K-1

Annealen
info via Simax

560 °C

Annealing consists of three phases:
1. Warming
2. Remaining at temperature (annealing) at the upper annealing temperature to reduce stress.
3. Temperature drop from the upper limit to the lower limit of annealing temperature and from there to the final ambient temperature.
Simax provides a specific annealing cycle in the table below.
Warming upAnnealingTemperature drop
Max. wall thickness20 - 550 °C560 °C560 - 490 °C490 - 440 °C440 - 40 °C
3 mm140 °C/min5 °C/min14 °C/min28 °C/min140 °C/min
6 mm30 °C/min10 °C/min3 °C/min6 °C/min30 °C/min
9 mm15 °C/min18 °C/min1.5 °C/min3 °C/min15 °C/min
12 mm8 °C/min30 °C/min0.6 °C/min1.6 °C/min8 °C/min